Table 1 Physical properties of the electrospun nanofibers

From: Sandwich-like electro-conductive polyurethane-based gelatin/soybean oil nanofibrous scaffolds with a targeted release of simvastatin for cardiac tissue engineering

Sample

Average fiber diameter

(nm)

Conductivity

(µs/cm)

Contact angel

(Ëš)

Young’s modulus

(Mp)

Ultimate tensile strength

(Mp)

Elongation at break

(%)

PGU

403 ± 119

9.55 × 10− 5

83 ± 3.40

10.00 ± 0.36

0.33 ± 0.04

3.45 ± 0.43

PGU-Soy

417 ± 167

0.54

61 ± 1.00

21.77 ± 0.20

0.72 ± 0.06

14.52 ± 0.47

PGU-Soy/G

361 ± 109

0.75

51 ± 1.37

12.25 ± 0.25

0.42 ± 0.02

15.00 ± 0.32

PGUSoy/GS

362 ± 83

0.80

33 ± 0.43

5.69 ± 0.28

0.43 ± 0.03

28.25 ± 0.26